Clarke AT162 ARC TIG/MMA Inverter Welder Instruction Manual
- June 6, 2024
- Clarke
Table of Contents
- INTRODUCTION
- SUITABILITY
- GUARANTEE
- UNPACKING
- GENERAL SAFETY INSTRUCTIONS
- SAFETY SYMBOLS
- ENVIRONMENTAL RECYCLING POLICY
- ELECTRICAL CONNECTIONS
- MMA/ARC WELDING
- STRIKING THE ARC-WELDING
- TIG WELDING
- WELDING PITFALLS
- TROUBLESHOOTING
- MAINTENANCE
- RATING PLATE
- DUTY CYCLE
- SPECIFICATIONS
- ACCESSORIES
- EXPLODED DIAGRAM & PARTS LIST AT162
- DECLARATION OF CONFORMITY-UKCA
- DECLARATION OF CONFORMITY-CE
- Read User Manual Online (PDF format)
- Download This Manual (PDF format)
WARNING: A suitable welding headshield must be worn during use
WARNING: Read these instructions before using the machine
ARC TIG/MMA WELDER
MODEL NO: AT162
PART NO: 6012145
OPERATION & MAINTENANCE
INSTRUCTIONS ORIGINAL INSTRUCTIONS
DL0821 – REV 3
INTRODUCTION
Before attempting to operate the machine, it is essential that you read this manual thoroughly and carefully follow all instructions given. In doing so you will ensure the safety of yourself and that of others around you, and you can also look forward to the welder giving you long and satisfactory service. The AT162 is designed to be used for both metal ARC (MMA) and TIG welding (TIG welding leads are not supplied with the machine. These are, however, readily available from your CLARKE dealer (Part number 6012233)).
SUITABILITY
MMA/Arc Welding | Carbon Steel, Low Alloy Steel, Stainless Steel, Cast Iron. |
---|---|
TIG Welding | Carbon Steel, Low Alloy Steel, Stainless Steel, Cast Iron, |
Titanium, Copper + Brass.
GUARANTEE
This CLARKE product is guaranteed against faulty manufacture for a period of
12 months from the date of purchase. Please keep your receipt as proof of
purchase.
This guarantee is invalid if the product is found to have been abused or
tampered with in any way, or not used for the purpose for which it was
intended.
Faulty goods should be returned to their place of purchase, no product can be
returned to us without prior permission.
This guarantee does not affect your statutory rights.
UNPACKING
Any damage or deficiency should be reported to your CLARKE dealer immediately. You should find inside the box the following:
- 1 x 160A ARC / TIG Inverter Welder
- 1 x Electrode Clamp & Cable
- 1 x Wire Brush / Hammer
- 1 x Earth Clamp & Cable
GENERAL SAFETY INSTRUCTIONS
WARNING: WHEN USING ELECTRICAL TOOLS, BASIC SAFETY PRECAUTIONS SHOULD
ALWAYS BE FOLLOWED TO REDUCE THE RISK OF FIRE, ELECTRIC SHOCK, AND PERSONAL
INJURY.
WARNING: READ ALL THESE INSTRUCTIONS BEFORE ATTEMPTING TO OPERATE THIS
PRODUCT AND KEEP THESE INSTRUCTIONS IN A SAFE PLACE.
ELECTRIC SHOCK
- Always remove the plug from the socket and wait 5 minutes to allow the capacitors to discharge before carrying out servicing or maintenance.
- Do not touch live electrical parts.
- Never use electrode holders or cables that are damaged.
- Keep the working environment, equipment, cables, and clothing free from grease, oil, moisture, and dirt.
- Ensure the welding machine has been correctly earthed.
- The operator must be insulated from the floor and workbench, using a dry insulation mat.
- Always ensure a second person is present in case of an accident.
- Never change electrodes with bare hands or damp gloves.
- Keep welding cables away from power cables.
- Regularly inspect the condition of the cables for signs of damage.
- Remove the plug from the main socket when not in use, do not leave the machine unattended.
- Ensure the earth clamp is secured to bare metal adjacent to the weld seam, and when not in use, is insulated for safety. – Keep all equipment well maintained.
- The operator shall prevent gas cylinders in the vicinity of the workpiece from becoming part of the welding circuit.
FUMES & GASES
- The welding process generates hazardous fumes as a by-product. Inhalation of these fumes is hazardous to health.
- Keep your head away from the weld to avoid breathing the fumes.
- If welding in confined spaces, ensure adequate ventilation and use a fume extractor.
- By-products of welding can react to create a toxic/explosive environment.
FIRE OR EXPLOSION
Welding can cause fires and explosions. Precautions should be taken to prevent
these hazards.
- Before starting work ensure the area is clear of flammable materials.
- Move any combustible materials to a safe distance, especially substances likely to generate a dangerous vapor.
- The welding arc can cause serious burns. Avoid contact with the skin.
- Sparks and molten metal are ejected during welding. Take precautions to prevent fire.
- Sparks and molten metal can pass through gaps. Be aware that fire can start out of sight.
- Do not weld pressurized containers. or containers containing flammable vapors e.g. fuel tanks.
- Always have appropriate fire fighting equipment to hand suitable for use in electrical environments.
- Avoid carrying any fuels with you e.g. cigarette lighters or matches.
PERSONAL PROTECTION
- The body should be protected by suitable clothing.
- The use of neck protection may be necessary against reflected radiation.
- Arc welding machines generate a magnetic field which is detrimental to pacemakers. Consult your doctor before going near active welding equipment/operations.
- The UV and IR radiation generated by welding is highly damaging to the eyes, causing burns. This can also affect the skin.
- Always use a suitable welding shield equipped with appropriate protective filters.
- Where there are pedestrians and traffic, ensure a protective screen is used to avoid accidental arc glare.
- Do not weld in the vicinity of children or animals and ensure no one is looking before striking an arc.
- Wear hearing protection if required.
- Allow the weld time to cool. Hot metal should never be handled without gloves.
- Take care when adjusting or maintaining the torch. Make sure it has had time to cool sufficiently and the welder is disconnected from the main supply.
- First aid facilities and a qualified first aid person should be available unless medical facilities are close by, for immediate treatment of flash burns of the eyes and for skin burns.
- A hard hat should be worn when others are working overhead.
- Flammable hair sprays/gels should not be used by persons intending to weld or cut.
PROTECTIVE CLOTHING
- Wear gauntlet gloves designed for use in welding.
- Wear an apron and protective shoes.
- Wear cuffless trousers to avoid entry of sparks and slag.
- Avoid oily, greasy clothing.
- Protective head and shoulder coverings should be worn when overhead welding.
- Wear a welding head shield with appropriate filter lenses or plates (protected by clear glass). This is a MUST for welding (and chipping) to protect the eyes from radiant energy and splatter. Replace cover glass when broken, pitted, or splattered.
NOTE: ALL protective wear inc. masks & head shields MUST comply with PPE Directive 89/686/EEC
ADDITIONAL SAFETY PRECAUTIONS FOR ARC WELDERS
- NEVER attempt to remove any of the exterior panels unless the machine is disconnected from the power supply.
- NEVER use the machine with any of the panels removed.
- NEVER attempt any electrical or mechanical repair unless you are a qualified technician. If you have a problem with the machine contact your local CLARKE dealer.
- NEVER use or store in a wet/damp environment. DO NOT EXPOSE TO RAIN.
- NEVER allow children or animals in the vicinity of a welding operation.
- ALWAYS remove all flammable materials from the welding area.
- ALWAYS ensure that there is full free air circulating around the outer casing of the machine and that the louvers are unobstructed.
- The welding arc can seriously damage your eyes. Both the operator and any spectators should always use a proper welding face shield or helmet, with suitable filter lenses. Proper gloves and working clothes should be worn at all times.
- ALWAYS wear a pair of safety spectacles/goggles when chipping away slag after welding. Remember, ordinary eyeglasses are not safety glasses.
- ALWAYS ensure there is a fire extinguisher on hand.
- ALWAYS ensure there is adequate ventilation or extraction in the work area, as the welding process gives off toxic fumes.
- ALWAYS ensure that a medical supply is on hand, and that treatment for burns is available.
SAFETY SYMBOLS
****| Read this instruction booklet carefully before use.| | Do not expose
to rain.
---|---|---|---
| Wear eye protection| | Recycle unwanted materials instead of disposing of
them as waste. All tools, accessories, and packaging should be sorted, taken
to a recycling center, and disposed of in a manner that is compatible with the
environment.
| Wear protective gloves
| Wear a dust mask
ENVIRONMENTAL RECYCLING POLICY
Through the purchase of this product, the customer is taking on the obligation
to deal with the WEEE in accordance with the WEEE regulations in relation to
the treatment, recycling & recovery, and environmentally sound disposal of
the WEEE.
In effect, this means that this product must not be disposed of with general
household waste. It must be disposed of according to the laws governing Waste
Electrical and Electronic Equipment (WEEE) at a recognized disposal facility.
ELECTRICAL CONNECTIONS
CONNECTING TO MAINS
NOTE: This tool is earthed and must only be connected to mains with an
earth connection. Do not attempt to use it without an earth connection.
- This welder is not supplied with a mains electrical plug because at full capacity it will draw far too much power for a normal domestic 230V mains plug and socket. This welder must not be fitted with a standard 13A UK plug.
- A high current 230V mains socket or terminal must be installed by a qualified and accredited professional electrician. A 16A socket and plug conforming to IEC 60309 is recommended.
- A non-socketed mains connection also requires a welder connection by a qualified and accredited professional electrician. However, a socketed connection is safer and more strongly recommended so the welder can be safely isolated when necessary. If directly wired to mains, a double pole, double throw isolator switch must be fitted.
- The welder must be connected to a consumer unit with a built-in RCD, using a circuit protected by an RCD.
- Please refer to the Specification for details of the maximum current required by this welder.
- If in any doubt, do not attempt to connect or use this welder until a professional electrician has been consulted.
MMA/ARC WELDING
A consumable electrode is connected to a high amperage low voltage supply
which creates an electric arc between the electrode and the workpiece.
Benefits over TIG welding include less experience needed, torch kit or
shielding gas are not required.
PREPARATION
- Arc welding cables are supplied with this machine.
To prepare the unit for ARC welding, it is important that you follow the
procedure below.
-
Making sure that the ON/OFF switch, located on the rear panel is in the OFF position, connect the welding leads as follows:
• Welding rod holder lead to the +ve terminal.
• Work clamp leads to the -ve terminal. -
Select the appropriate welding rod and insert it into the welding rod holder• The size (diameter) of the welding rod should be approximately the same as the thickness of metal to be welded.
-
Attach the work clamp to the workpiece as close as possible to the area being welded. Clean with a wire brush where necessary to ensure the connection is as clean as possible.
-
Set the required current using the current selector.
• With practice you will gain a feel for the correct current setting for different welding rod thicknesses.
• The following table gives a useful guideline.
Material Thickness| Welding Rod Size| Current (Amps)
---|---|---
1-2 mm| 2.5 mm| 70 – 100
2-5 mm| 3.2 mm| 100 – 125
5-8 mm| 4.0 mm| 125 – 160 -
Switch ON using the switch located on the rear panel.
• The green light on the front panel should glow, indicating the machine is ON.
• If the machine stops at any time and the amber light comes ON, the thermal overload device has intervened. Wait until the welder has cooled sufficiently (the amber light goes out) before restarting work.
STRIKING THE ARC-WELDING
WARNING: WHEN WELDING ALWAYS ENSURE THERE IS ADEQUATE VENTILATION IN THE
WORK AREA AS THE WELDING PROCESS GIVES OFF TOXIC FUMES.
WARNING: ALWAYS USE A SUITABLE WELDING MASK OR SHIELD WHEN USING ANY
WELDER.
The most difficult aspect of the arc welding process, particularly for beginners, is that of striking an arc. We strongly recommend that you practice on some pieces of scrap metal to get the feel of the operation before you start on an actual welding job.
-
Hold the electrode about 10 mm from the work and at an angle of about 70° to 80° to the work surface; take care not to accidentally touch the workpiece until you are ready to start.
-
Holding the welding mask close-up to your face, give a short stroke with the electrode on the workpiece. As soon as the arc is primed, withdraw the electrode from the workpiece to leave a tiny gap of around 1.5mm (1/16″). The current will flow across the gap with a crackling noise and a brilliant arc. Continue to weld in one direction, maintaining the small gap as you go.
NOTE: When you prime the arc, be sure to withdraw the electrode swiftly to leave the 1.5 mm. gap, otherwise the electrode will weld itself to the workpiece. If this occurs give the electrode a short sharp jerk to free it and, if necessary, prime the arc again. If you cannot free the electrode, switch the machine off immediately and free it. Take care the electrode will get red hot very quickly and will be capable of burning through welding gloves. -
At the end of the run, just lift the electrode away from the workpiece.
• Inspect the job carefully. Any slag forming on the surface should be chipped away with a chipping hammer or pick. ALWAYS wear your safety goggles when chipping away slag.
TIG WELDING
TIG welding is primarily for very thin materials. It uses a non-consumable
tungsten (or tungsten alloy) electrode, held in a torch.
A shielding gas (100% Argon), is fed through the torch to protect:
• The electrode,
• Molten weld pool,
• Solidifying weld metal from contamination by the atmosphere.
The electric arc is produced by the passage of current through the conductive,
ionized shielding gas. The arc is established between the tip of the electrode
and the work. The heat generated by the arc melts the base metal. Once the arc
and weld pool is established, the torch is moved along the joint and the arc
progressively melts the joined surfaces. Filler wire, if used, is usually
added to the leading edge of the weld pool to fill the joint. This process is
ideally suited for welding thin metals such as car body panels, pressure
vessels, heat exchangers, pipes, etc., where accuracy and a high-quality weld
are desired, as it produces a very low porosity weld.
MAIN FEATURES OF TIG WELDING
- Electronic control of welding current.
- Forced air cooling.
- A thermal overload protection device prevents overheating.
TIG WELDING PROCESS ADVANTAGES
- It produces superior quality welds, generally free of defects.
- It is free of the spatter which occurs with other arc welding processes.
- It can be used with or without filler metal as required.
- It allows excellent control of root pass weld penetration.
- It can produce welds at high speeds.
- It allows precise control of the welding variables.
- It is capable of welding very thin material (0.5mm), without undue distortion.
LIMITATIONS
- Greater weld dexterity is required.
- These units have a DC output that is not suitable for welding aluminum.
TIG WELDING (REF FIG.2)
- The machine is not equipped with a TIG welding torch and cables; these are available from your Clarke dealer (Part number 6012232).
- Additionally, before TIG welding, you must obtain a gas cylinder of 100% pure Argon.
To prepare the unit for TIG welding, it is important that you adopt the following procedure.
-
Plug the work clamp lead into the +ve terminal, and secure the work clamp to the workpiece.
• For good contact, the work clamp must be attached to clean bare metal. Clean with a wire brush where necessary. -
Plug the torch lead to the -ve terminal.
-
Screw the pressure regulator onto the gas bottle tightly, and attach the gas hose to the inlet connector securely, with a hose clip.
-
Turn the pressure regulator knob to set a pressure of approx. 2.5kg/ cm2(35 lb/in 2 ).
-
Ensure the electrode at the torch nozzle protrudes by 4 – 5mm, also ensure that the electrode is sharply pointed with an angle of 40°-60°, if it is not, grind it to shape. (Consult your TIG Torch manual for the procedure for adjusting the electrode).
-
Set the welding current in accordance with the thickness of the material to be welded and the size of the tungsten electrode to be used, (See page 13).
-
Switch ON using the switch mounted on the rear panel. The green light on the front panel will glow.
• If the machine stops at any time and the amber light comes ON, the thermal overload has intervened. Wait until the welder has cooled sufficiently (the amber light goes out) before restarting work. -
Open the gas valve on the torch handle,
• This will allow gas to flow from the torch nozzle. -
Cover your face with the head shield, bring the torch to within 3-4mm of the work, and at an angle of 45°, so that the ceramic nozzle gently touches the work surface. See fig. 3.
-
Scratch the tip of the electrode against the piece to be welded, as soon as the welding arc starts, remove the electrode to a distance of 3-4 mm, and continue the weld. (See notes below).
• This method is referred to as ‘Scratch Arc’. -
To stop welding, simply remove the torch from the workpiece.
-
Turn OFF the gas as soon as you finish welding.
NOTE:
- To avoid a visible strike mark on the surface of the workpiece, it is advisable to strike the arc in the joint, where the mark will be concealed by the weld.
- Thin sheet and stainless steel may be welded with or without filler, similar to gas welding.
- The filler is fed in at the edge of the pool. The rod must not touch the tip of the electrode or enter the arc. The end of the rod must always be shielded by the argon atmosphere to prevent as far as possible the formation of oxides on its surface. When welding stainless steel and copper, it is often possible to feed in the filler continuously at the edge of the pool.
- The arc length generally varies between 3 and 6 mm depending on the type of joint, type and thickness of the material, and so on.
- The torch is advanced in the direction of welding, without lateral movement, maintaining the torch angle of 45° to the workpiece.
- Guidelines for the TIG welding current needed and recommended electrode sizes etc. for different gauges of material are shown in the chart below:
Metal| Welding Current (Amps)| Workpiece Thickness
(mm)| Filler Rod Dia (mm)| Welding Electrode Dia (mm)| Gas
Flow ltr/min
---|---|---|---|---|---
Mild Steel| 20-30| 1| 0-1| 1.6| 4-5
60-80| 2| 1.2-1.6| 1.6| 4-5
80-110| 3| 1.6-2.0| 1.6/2.4| 4-5
100-130| 3.5| 2.0-2.4| 2.4| 5-6
130-140| 4| 2.4| 2.4| 6-7
140-150| 4.5| 2.4| 2.4| 7-8
150-160| 5| 2.4| 2.4| 7-8
Stainless Steel| 15-35| 1| 0-1| 1.6| 4-5
60-80| 2| 1.2-1.6| 2.4| 4-5
80-115| 3| 1.6-2.0| 1.6/2.4| 4-5
100-130| 3.5| 2.0-2.4| 2.4| 5-6
130-140| 4| 2.4| 2.4| 6-7
140-150| 4.5| 2.4| 2.4| 7-8
150-160| 5| 2.4| 2.4| 7-8
Copper| 80| 2| 2.0| 1.6| 5-6
125| 3| 2.4| 2.4| 5-6
135-150| 4| 2.4| 2.4| 6-7
150-160| 4.5| 2.4| 2.4| 7-8
WELDING PITFALLS
The arc welding technique is an acquired skill and requires considerable practice before perfect results are obtained. The diagrams below will help to explain the pitfalls in your technique and how to overcome them.
ARC TOO SHORT
This causes irregular masses of weld to be deposited, with slag contamination
on an uneven surface.
ARC TOO LONG
This causes poor penetration resulting in a weak weld with excessive spatter
and porosity. The surface of the weld is rough and the arc makes a hissing
sound
E LECTRODE MOVED TOO SLOWLY
This causes a very wide and heavy deposit that overlaps at the sides. It is
wasteful both in terms of time and electrode use.
ELECTRODE MOVED TOO QUICKLY
This causes poor penetration with a ‘stringy’ and incomplete weld deposit.
Slag is very hard to remove.
CURRENT TOO LOW
This causes poor penetration and causes the electrode to stick to the
workpiece too readily. Also results in a very irregular and high weld deposit.
Slag is very hard to remove.
CURRENT TOO HIGH
This causes excessive penetration with spatter and deep pointed crater. It may
also cause holes to be burned in the workpiece.
Burns electrodes very quickly.
THE PERFECT WELD
With the correct combination of arc length, current regulation, inclination,
and speed of the electrode, you will, with practice, produce the perfect weld.
This should be regular with uniform ripples and no slag contamination. The arc
will make a steady crackling sound.
TROUBLESHOOTING
DEFECT
| CAUSES|
SUGGESTIONS
---|---|---
Spark will not start| Bad clamp connection. Inverter printed circuit is
defective.| Check clamp connection. Contact your nearest CLARKE dealer.
No output voltage| Overheated machine (the yellow LED should be on).| Wait for
the thermal cutout to be reset.
Under-voltage/over-voltage limits exceeded. Yellow LED on and green LED
flashing.| Check the mains distribution system.
Wait for an internal check of input voltage. When this is within normal limits, the yellow LED will go out and the green LED will stay on.
The internal relay has failed.| Contact your nearest CLARKE dealer.
Inverter printed circuit is defective.| Contact your nearest CLARKE dealer.
Wrong output current| The current selector control is defective.| Contact your
nearest CLARKE dealer.
Low power supply voltage.| Check the mains distribution system.
Porosity of welds| The acid electrode on steel with high sulfur content.
Electrode oscillates too much.
Workpieces are too far apart.
The workpiece being welded is cold.
| Use basic electrodes.
Move edges to be welded closer together. Move slowly at the beginning.
Cracks in weld| The material being welded is dirty (e.g.oil, paint, rust, oxides).
Not enough current.
| Clean workpiece before welding is an essential method of achieving neat weld
beads.
Limited penetration| Low current, high welding rate, reversed polarity.
Electrode inclined in position opposite to its movement.
| Ensure operating parameters are regulated and improve the preparation of workpieces.
DEFECT
| CAUSES|
SUGGESTIONS
---|---|---
High Sprays| The electrode is too inclined.| Make appropriate corrections.
Profile defects.| Welding parameters are incorrect. The pass rate is not
related to operating parameter requirements. Electrode not inclined constantly
while welding.| Follow basic and general welding principles.
Arc is unstable.| Insufficient current.| Check the condition of electrode and
earth wire connection.
Electrode melts| The electrode core is not centered. Magnetic blow
phenomenon.| Replace electrode. Connect two earth wires to opposite sites of
the workpiece.
MAINTENANCE
WARNING: DISCONNECT FROM MAINS BEFORE CLEANING.
WARNING: DO NOT ATTEMPT TO CARRY OUT REPAIRS YOURSELF, UNLESS YOU ARE FULLY COMPETENT, ALL WORK MUST BE CARRIED OUT BY A QUALIFIED TECHNICIAN.
The welder requires very little maintenance other than the following guidelines. Under normal working conditions removing the covers and cleaning with dry compressed air at reduced pressure once a year will be quite sufficient. Cleaning at more frequent intervals is advisable, however, if the unit is operating in a dusty and dirty environment.
- Keep the louvers clean to avoid a build-up of dirt and oxides inside the machine, which can reduce machine output.
- Check all cables periodically for condition and security. They must be in good condition and not cracked.
- Always avoid getting particles of metal inside the machine since they could cause short circuits.
RATING PLATE
1 | Name and address of the manufacturer | 12 | Rated Welding Current Symbol |
---|---|---|---|
2 | Model Number, / Part Number | 13 | Conventional Load Voltage Symbol |
3 | Serial / Batch Number | 14 | Energy Supply Symbol |
4 | Welding Power Source | 15 | Rated Supply Voltage |
5 | British Standards applied | 16 | Rated Maximum Supply Current |
6 | Welding Process Symbol | 17 | Maximum Effective Supply Current |
7 | This symbol indicates that the unit is suitable for carrying out welding | ||
operations in an environment that has an increased risk of electric shock. | |||
18 | N/A | ||
8 | Welding Current Symbol | 19 | N/A |
9 | Rated No-load Voltage | 20 | N/A |
10 | Range Of Output | 21 | N/A |
11 | Duty Cycle Symbol | 22 | Degree of Protection |
DUTY CYCLE
This welder is covered by regulations BS EN 60974-1:2012, where the Duty Cycle (X) is expressed as a percentage of time the machine may be used in a given period for a specified welding current. i.e. When welding at 100 Amps the machine may be used for 6 minutes (60%) in any10 minute period,
SPECIFICATIONS
| AT162
---|---
Unpacked Weight (kg)| 5.7
Dimensions (l x w x h) (mm)| 300 x 132 x 212
Power Supply| 230V AC~ 50Hz
Rated Max Input Current (A) I1Max / I1eff(A)| 33 / 15.8
No Load Voltage (V)| Uo=85V
Max/Min Welding Current (A)| 10A/160A
IP Rating| IP21S
Suitable Electrodes (mm)| 2.5 + 3.2 +4.0
NOTE: The details and specifications contained herein, are correct at the time of going to print. However, CLARKE International reserve the right to change specifications at any time without prior notice.
ACCESSORIES
The following are some of the accessories available from your CLARKE dealer.
Please quote the part numbers shown below:
DESCRIPTION | PART NUMBER |
---|---|
Range of Arc Activated Welding Headshield | See Your Clarke Dealer |
2.5 mm Arc Welding Electrodes | 3050584 |
3.2 mm Arc Welding Electrodes | 3050586 |
4.0 mm Arc Welding Electrodes | 3050588 |
TIG Welding Torch Assembly (AT162, AT165) | 6012233 |
Argon Gas Regulator | 8134140 |
EXPLODED DIAGRAM & PARTS LIST AT162
NO | DESCRIPTION | NO | DESCRIPTION |
---|---|---|---|
1 | Handle | 14 | Inductance |
2 | Top Housing | 15 | Temi160 rectifier radiator |
3 | Switch | 16 | Fast recovery diode |
4 | Cable Gland | 17 | Control PCB |
5 | Fan Hood | 18 | Main PCB |
6 | Power Cable | 19 | Base Frame |
7 | Fan | 20 | Rubber Foot |
8 | Bridge Heatsink | 21 | Quick connector ASM |
9 | IGBT Radiator | 22 | Knob |
10 | Support bar | 23 | Digital Display |
11 | Rectifier bridge | 24 | Shade |
12 | IGBT | 25 | Power Controller |
13 | Transformer |
DECLARATION OF CONFORMITY-UKCA
DECLARATION OF CONFORMITY-CE
PARTS & SERVICE:
0208 988 7400
Parts Enquiries
Parts@clarkeinternational.com
Servicing & Technical Enquiries
Service@clarkeinternational.com
SALES: UK 01992 565333 or Export 00 44 (0)1992 565335
Clarke INTERNATIONAL Hernnall Street, Epping, Essex CM16 4LG
www.clarkeinternational.com
Read User Manual Online (PDF format)